Material Compatibility Chart: Carbon Steel, 304, 316, Duplex, Super Duplex, Alloy 625, C-276, Titanium and More Against 42 Fluids

Material selection for a sour-gas separator, a seawater cooler, an acid dosing skid or a caustic tank starts with the same question: which alloy survives this fluid at this temperature? This chart answers it for eighteen materials, from carbon steel and 304 stainless through 316, lean, standard and super duplex, the super-austenitic and nickel families to titanium, against 42 of the media our customers specify. Choose the medium to rank the alloys, choose the alloy to see its strengths and weaknesses, or open the full matrix.
How to read it
A to D are screening ratings for the condition band named in the medium (dilute, concentrated, ambient, hot, aerated, deaerated). Within a band the exact concentration, temperature, velocity, aeration and impurities decide, which is why every C is a "test first".
PREN (pitting resistance equivalent, Cr + 3.3 Mo + 16 N) ranks stainless, duplex and Ni-Cr-Mo alloys for chloride pitting and crevice corrosion: about 24 for 316L, 35 for 2205 and 904L, 42 to 43 for super duplex and 6Mo, 51 for Alloy 625 and above 65 for C-276 and C-22. It says nothing about acids, caustic or high temperature.
Sour service notes refer to NACE MR0175 / ISO 15156-3, which lists each alloy with environmental limits (H2S partial pressure, chloride, temperature, pH) and hardness limits; an "A" in wet H2S assumes the alloy is used within those limits. See our NACE MR0175 guide.
Oxidising or reducing is the first question for acids: molybdenum-rich alloys (B-2, C-276) win in reducing acids such as hydrochloric; chromium-rich alloys (stainless, C-22, titanium) win in oxidising acids such as nitric. A few parts per million of Fe³⁺ or Cu²⁺ turns a reducing acid oxidising and changes the answer.
Where the chart is usually decisive
Carbon steel first: it is the default wherever a corrosion allowance, coating or inhibitor makes it last; the chart shows where it does not (aerated chlorides, dilute acids, deionised water) and where it surprisingly does (concentrated sulphuric acid, anhydrous HF, dry chlorine, caustic at ambient).
304 versus 316: molybdenum buys 316 its chloride resistance; 304L keeps the edge in hot nitric acid. Neither survives seawater.
Seawater and produced water: 316L pits under deposits; 2205 crevice-corrodes above about 20 °C; 6Mo, super duplex, Alloy 625, C-276 and titanium are the working choices, and the budget decides between a super-duplex shell and a titanium tube bundle.
Sour gas: Alloy 825 cladding and tubing, super duplex within its H2S limits, Alloy 625 and C-276 for the worst wells; carbon steel with inhibition where the economics allow.
Hydrochloric acid: Alloy B-2 (deaerated) and C-276; nothing in the stainless family.
Sulphuric acid: Alloy 20, 904L and 825 in the dilute range; concentrated acid is a different problem with its own alloys.
Caustic: stainless to about 90 °C, then nickel 200/201 or Alloy 400.
Chlorine and hypochlorite: titanium in wet chlorine and bleach, never in dry chlorine; C-276 across both.
Hydrofluoric acid: Alloy 400, with C-276 and 625 for limited duties.
High temperature: Alloy 800H and 625 for furnaces and reformers; duplex stainless stops at about 280 °C.
What we build in these alloys
Special-alloy process vessels, special-alloy replacement tube bundles, super-duplex seawater coolers, special-alloy static mixers, HF acid vaporisers and condensers, sour-gas autoclaves and sour-service corrosion test kits for the coupon and autoclave tests that confirm a rating on your own fluid. Related guides: ISO 21457 materials selection, NACE TM0177 and TM0284 sour-service testing, ASTM G48 pitting and crevice test, EN 10204 material certificates. All Tech Inc. calculators and converters.
Write to mail@techincresearch.com or call +1 (289) 622-1032.
Disclaimer: this calculator and article give estimates from simplified, published equations and the values you enter, for general information only and without warranty. They are not engineering, design, safety or regulatory advice and are no substitute for measurement, the equipment or chemical maker's instructions, the applicable standards or the judgement of a qualified engineer. Do not rely on them for safety-critical decisions. Tech Inc. accepts no liability for loss, damage or injury arising from their use. Equipment specifications are typical and may change; results depend on the fluids and conditions, how the equipment is used and operation in line with the operation manual. See our product information disclaimer and terms of use.
Sources
AMPP (formerly NACE International), ampp.org, publisher of NACE MR0175 / ISO 15156 and the corrosion survey data behind generic compatibility ratings.
International Molybdenum Association, Duplex stainless steels, PREN and duplex service limits.
ASTM International, ASTM G48 Standard Test Methods for Pitting and Crevice Corrosion Resistance of Stainless Steels and Related Alloys by Use of Ferric Chloride Solution, standard summary page.





Comments