Galvanic Series Chart for Seawater: Which Metal Corrodes When Two Are Coupled, with Potentials and Area Ratio

Every mixed-metal assembly in seawater, brine or chlorinated cooling water is a battery. The more active member corrodes to protect the nobler one, and the rate depends on how far apart the two sit in the galvanic series and on the ratio of their areas. This chart places 41 common metals and alloys on the series, from graphite and titanium at the noble end to zinc and magnesium at the active end, and tells you for any couple which member is the anode, how large the potential difference is and whether the couple needs isolation, coating or a sacrificial anode.
How to read it
Potentials are typical ranges in flowing aerated seawater at about 25 °C, measured against a saturated calomel electrode, as published in the galvanic series that accompanies ASTM G82 and similar compilations. Other electrolytes shift the values; the order is what matters.
The anode corrodes. Current flows from the less noble (more negative) member; its corrosion rate rises with the potential difference and with the cathode-to-anode area ratio. A stainless bolt in a steel flange is safe (small cathode); a steel bolt in a stainless flange is not.
Stainless steel has two positions. Passive 304 and 316 sit near the nickel alloys; inside a crevice or under a deposit the same steel is active and sits with the carbon steels. Every crevice-corrosion failure of a stainless tube bundle is this chart in action.
Severity bands (negligible below 0.05 V; acceptable to 0.15 V in seawater, 0.25 V in normal atmospheres, 0.50 V in dry conditions) are the usual engineering rule of thumb, not a standard.
What the chart settles on a skid
Titanium tube bundles in copper-alloy or steel shells need the shell protected: the bundle is a very efficient cathode.
Super duplex and 6Mo coolers with carbon steel piping need isolation flanges or the steel takes the hit at the joint.
Aluminium instrument housings and junction boxes on stainless skids corrode at the mounting feet; isolate with nylon washers and sleeves.
Graphite gaskets and packing against any metal in seawater are the worst couple on the chart; use PTFE or non-conductive fibre.
Sacrificial anodes are chosen from the bottom of the series: zinc or aluminium for steel in seawater, magnesium in fresh water and soil. See our NACE SP0169 cathodic protection guide.
Our equipment
Super-duplex seawater coolers, special-alloy replacement tube bundles, hairpin heat exchangers, aquaculture oxygenation skids, produced water treatment packages and corrosion monitoring access fittings. Related: material compatibility chart and ISO 21457 materials selection. All Tech Inc. calculators and converters.
Write to mail@techincresearch.com or call +1 (289) 622-1032.
Disclaimer: this calculator and article give estimates from simplified, published equations and the values you enter, for general information only and without warranty. They are not engineering, design, safety or regulatory advice and are no substitute for measurement, the equipment or chemical maker's instructions, the applicable standards or the judgement of a qualified engineer. Do not rely on them for safety-critical decisions. Tech Inc. accepts no liability for loss, damage or injury arising from their use. Equipment specifications are typical and may change; results depend on the fluids and conditions, how the equipment is used and operation in line with the operation manual. See our product information disclaimer and terms of use.
Sources
ASTM International, ASTM G82 Standard Guide for Development and Use of a Galvanic Series for Predicting Galvanic Corrosion Performance, standard summary page.
AMPP (formerly NACE International), ampp.org, corrosion reference material.