Process Note: Sour-Service Materials Testing in Autoclaves

At a glance. Hydrogen sulphide (H2S) in oil and gas production lets atomic hydrogen enter steel. This can cause sulphide stress cracking (SSC), hydrogen-induced cracking (HIC) and stress-oriented hydrogen-induced cracking. ISO 15156, also published as NACE MR0175, sets out how materials are qualified for these conditions, and NACE (now AMPP) test methods define the laboratory tests. Laboratories across the world, at operators, steel makers, pipe mills and research institutes, run these tests at atmospheric pressure in glass vessels or, for field-specific conditions, in autoclaves at higher H2S partial pressures and temperatures.
The main tests
NACE TM0177 covers SSC testing, with Method A (uniaxial tensile), Method B (bent beam), Method C (C-ring) and Method D (double cantilever beam). Methods A to C typically run for 720 hours.
NACE TM0284 covers HIC testing of pipeline and pressure vessel steels. Unstressed specimens are exposed for 96 hours, then sectioned to measure the crack length, thickness and sensitivity ratios (CLR, CTR and CSR).
Fit-for-purpose testing sets the test environment to match the expected field conditions: H2S and CO2 partial pressures, temperature, pH and chloride. Where the H2S partial pressure is above one atmosphere or the temperature is high, these tests need autoclaves. European Federation of Corrosion publications 16 and 17 give guidance for such tests.
The test process
Specimen preparation: machining, surface finishing and, for some methods, stressing in fixtures.
Solution preparation and deaeration with nitrogen, as oxygen distorts the results.
Gas saturation with H2S or an H2S and CO2 mixture at the test partial pressure.
Exposure at controlled temperature and pressure, with pH monitored.
Inspection: visual and magnified examination for cracks, sectioning and metallography, and crack measurement for HIC.
Safe disposal of H2S through scrubbers.
Design points for autoclave testing
Materials of construction, often nickel alloys such as Alloy C-276 for chloride and H2S service.
Pressure and temperature ratings that cover the whole test matrix.
Gas handling: a closed H2S supply, mixing, purging and scrubbing.
Load application inside the vessel, for example proof rings or constant-load fixtures.
Monitoring of temperature and pressure and, where possible, pH and H2S concentration.
Safety: H2S detection, ventilation, interlocks and emergency procedures, as H2S is lethal at low concentrations.
Common problems
Oxygen contamination, which changes corrosion and cracking behaviour.
H2S depletion during long tests unless the gas is replenished.
Leaks at fittings and seals, a serious hazard with H2S.
Crevice or galvanic effects from fixtures made of other materials.
Results that do not reflect the field because the test pH or partial pressure was set without care.
Where Tech Inc. equipment fits
Tech Inc. supplies the sour-gas autoclave for H2S service, the benchtop stirred high-pressure reactor in Alloy C-276, gas sampling panels for process, natural and sour gas, sampling cabinets for H2S and moisture analysers and, for field monitoring, corrosion monitoring access fittings and injection quills. The wider range is on our high-pressure reactors page.
Related reading
This note is general guidance. Test methods, acceptance criteria and safety procedures follow the applicable standards and the laboratory's own risk assessment.